We are a small fab shop that performs various welding repairs and fabrications for local farmers and construction companies, and occasionally we do some larger jobs for bigger companies. We typically weld everything with flux-cored or solid wire and some TIG welding. Recently, we ran out of our standard E71 flux-cored wire, but we had some E110 wire on hand from a previous job. We welded several mild steel parts with single- and multiple-pass welds with the E110 wire and experienced cracking in the base material next to the multipass welds. What would cause that to happen?
There are a few possible causes. However, the main reason is an overmatched filler metal strength compared to the strength of the base material. To understand why this happens, let’s clarify a few details.
You stated the base material that cracked was mild steel. Mild steels can have a range of mechanical properties, but most will have a yield strength of around 36 KSI (or 36,000 lbs. per square inch), and the ultimate tensile strength (UTS) range will be approximately 58 to 80 KSI.
The filler metal you used to weld the base material is an E110T-XX classification, with a minimum UTS of 110 KSI. As you can see, the filler metal has a much greater UTS than the base material.
The molten weld pool expands during welding, but when it cools and solidifies, there is a small percentage of contraction and shrinkage that produces significant internal weld stresses. These internal stresses are transferred directly to the adjacent base material. When the filler metal has a much higher UTS than the base material, the internal weld stresses overpower the base material, leading to cracking. This is why engineers usually match filler metal strength to the lower-strength base material in situations where a low- and high-strength base material are being joined.
You mentioned that the cracking occurred on the multipass welds but not on the single-pass welds. The first pass of any weld will have a percentage of base material dilution that will change the chemistry of the weld metal, which will lead to a change in mechanical properties. In the FCAW process, dilution may be as high as 30%, depending on joint design that, when mixed with the lower-strength base material, reduces the overall strength of the weld metal and works in your favor. However, the base material dilution percentage reduces significantly during multipass welds, because you are welding into the previously deposited layer. Dilution becomes a nonfactor as layers increase, which means that the weld metal will be at its classified strength—the residual stresses of the high-strength weld metal result in base material cracking.
The other potential causes for weld cracking in this scenario include failing to preheat, applying preheat temperatures that are too low for 1-in.-thick material, an overconstrained weld joint (too many braces or supporting members), or an improper shielding gas used with the FCAW process.
Technical Liaison
ESAB Welding & Cutting Products
Email Martin Denault
See More by Martin Denault
Senior Application Engineer, AWS – CWI, CWS, CWE
2800 Airport Road
Denton, TX 76207
See More by Robert Koltz
View the Digital Edition
Find The Welder on Facebook
Metal artist and fabricator Luis Varela-Rico joins The Fabricator Podcast to discuss his journey from union elevator mechanic…
Management FabCast Series 2026
FMA Annual Meeting 2027