Tube breakage has almost as many causes as there are tubes to be broken. Assessing the particulars takes a careful evaluation of dies, mandrels, material specs, and weld seam location. Jay Robinson
“Our tube is breaking, what do we do?”
Tube breakage along the outside radius of the bend is one of the most common issues in rotary draw tube bending. Sometimes, it is one of the hardest problems to diagnose.
This issue really boils down to two factors:
Here are some examples of recent customer problems and how we addressed them.
Motor Slippage and PDA Drift
One of our customers, an automotive exhaust manufacturer, would get through tool setup and make good parts. But after the part was in production for a while, the shop got random breaks in the tube. As time went on, the breaks became more frequent until nearly every bent part broke along the outside radius.
At this point, the shop would shut down production, lock out the machine, and double-check its tool setup. Not finding anything, the operator would restart, home the machine, and get back to good parts without having changed anything.
This was an all-electric machine, and the pressure die assist (PDA) (sometimes called a follower) was driven by a servomotor attached to a gear reducer that in turn drove the PDA forward via a rack and pinion gear setup. Because of the tight radius, the PDA was required to boost, or force, more material into the outside radius of the part. During bending, the shaft of the motor slipped in the coupler where it connected to the gear reducer, so after every bend, the position feedback from the servomotor indicated that the PDA was just a little bit farther forward than it actually was. So, every time it returned to its 0.00 position, the PDA would end up just a little bit behind where its 0.00 actually should have been.
Over time, the PDA would drift far enough back that there was not enough support along the outside radius at the beginning of the bend. That, coupled with the fact that the PDA was not pushing as much material to the outside radius as it could have been, resulted in progressively more breaks. When the process shut down and rehomed, the PDA would be reset to its correct position and the process would start over.
The breakage here was caused by excessive elongation due to a mechanical problem with the machine. To fix it, we retorqued the coupler in the gear box and had the shop change its program to reduce the torque output from the servomotor.
Without the motor slipping in the coupler, the PDA was able to do its job—forcing more material into the outside radius of the bend and reducing the amount the tube needed to elongate in the outside radius—more effectively.
Mandrel Misplacement and Clamp Slippage
In another instance, we had a client bending tube over a mandrel for an assembly that was a visible part of a final assembly.
The shop’s customer was very concerned about the appearance of the finished part, wanted no tool marks, and had a specific tolerance for the tube OD throughout the bend. The customer especially did not want the outside of the tube to appear flat or collapsed.
These specifications caused two problems, both resulting in broken tubes.
First, to reduce tool marks, the shop did not set up its clamp die as tightly as it normally would. As a result, during bending, the tube slipped in the clamp, and the tube was no longer being drawn into the bend die. Usually, we think this will cause wrinkles on the inside radius as the material tries to get “thicker” on the inside, but in this case, the tube was being stretched beyond its ability to elongate along the outside radius. Additionally, with the tube slipping through the clamp, the dies were making more tool marks than they would have with the clamps set properly. Once we had the clamps set up without slipping, the part was still breaking, but the break occurred several degrees deeper into the bend.
Using a set of calipers, we checked the outside radius of the part at a point just before the break. The company did not want to make a change because it had almost no reduction in OD—the outside radius, at least to the point of breakage, appeared perfectly round.
Double-checking the specified tolerance, we moved the mandrel back a little at a time, getting a little farther into the bend each time. Ultimately, we moved the mandrel back to a point where the shop could successfully complete the bend.
And even though the outside was not perfect, by allowing the tube to collapse to the low end of the tolerance, the team was able to produce bent parts that the customer would accept. The loose clamps were causing breakage because the tube was stretching more than the material could withstand. The mandrel was too far forward, the clamps were slipping, and both caused the material to thin excessively along the outside radius.
Elongation Exceeding Material Tolerance
A final example was a part that our customer had run many times previously. But suddenly, the shop could not produce a single bend without breaking the tube around the 15-degree mark.
The people at this shop used every trick they knew. They tried everything I suggested, too, but we made almost no improvement. A bit desperate to help our customer find a solution, I asked for the specification sheets that the mill provided when the tubing was purchased.
Tubing standards cover a wide array of specifications, from what materials are used (in specific percentages) to tolerances on the OD, ID, and wall thickness. One of the specifications is “elongation.” This value is expressed as a percentage.