A discussion of electric stick-out and contact-tip-to-work distance

Electrical stick-out and contact-tip-to-work distance are not the same thing, but they both play a role in welding a quality joint. rusak/iStock/Getty Images Plus

I have a general question. We use many welding procedure specifications (WPSs) that have been written by multiple people over the years. Some use the term ESO, or electrical stick-out, and others use CTTWD, which is contact-tip-to-work distance. I’ve asked the welders and some quality folks, and everyone tells me they mean the same thing. Why the different terms?

They are different terms because, by definition, they represent different things. This is a common mix-up throughout the welding industry.

These two terms describe measurements for the gas metal arc welding (GMAW), flux core arc welding (FCAW), and submerged arc welding (SAW) processes.

CTTWD is a straightforward measurement between the contact tip and the surface of the intended weld joint. Keep in mind that if you are welding in a deep groove weld, you need to measure to the bottom of the groove weld where the weld metal is deposited.

For most GMAW and FCAW applications, this measurement falls between 5/8 and 1 in. If you are using a large FCAW wire such as 3/32 in. dia., that distance can approach 1.5 to 1.75 in. If you are welding with the SAW process, the general rule of thumb is eight times the wire diameter, but typically never less than ¾ to 1 in.

ESO, on the other hand, measures the distance from the top of the welding arc to the contact tip. For obvious reasons, this is extremely difficult to measure. You might ask, then, why use it at all? This is where you can optimize your welding parameters or leverage welding circuit theory.

The total distance, or CTTWD, minus the ESO leaves the remaining distance as your arc length, which is your voltage. This information might come in handy, even if it doesn’t seem obvious at first.

When you are welding with GMAW or FCAW, you usually use a constant-voltage (CV) power supply. For these machines, you set your voltage and desired wire feed speed (WFS). WFS is fixed and constant, and the machine does whatever it can to maintain your set voltage. Your CTTWD determines the machine’s output amperage. The longer the CTTWD, the lower the amperage required to melt the filler metal. Conversely, the shorter the CTTWD, the higher the necessary amperage to melt the filler metal. This is due to Ohm’s law and resistive heating in the wire.

A way to think about this is to pretend the ESO portion of the wire is a fuse in an electrical circuit. We know that current flowing through a conductor, such as a wire, cable, filler metal, or a fuse produces heat due to resistance to flow. When the ESO is increased, it’s like using a smaller fuse in a circuit, so it takes less amperage to burn that fuse (i.e., your filler metal). If you shorten your ESO, you lose the preheating effect, and it takes more amperage to melt the filler metal. Similarly, it’s like installing a larger fuse that requires more amperage to melt it.

Welders who have discovered this phenomenon likely have tried shortening their ESO to increase amperage and penetration, or they use a longer ESO to reduce amperage and prevent blowing a hole through their workpiece, such as when they are welding on a weld joint with some small gaps.

For the SAW process, it is commonplace to maintain a steady amperage to produce a consistent depth of penetration or weld metal deposition rate. For this application, the machine control mode is set to constant amperage (CA), also referred to as constant current (CC). This means the operator sets a desired amperage and voltage, and the machine varies the WFS to maintain them. In this scenario, if the CTTWD is not consistent, variations in deposition rates occurs. A longer CTTWD increases WFS to maintain voltage and amperage, thereby increasing deposition rates. Conversely, a shorter CTTWD reduces WFS and reduces deposition rates. Therefore, in these applications that are highly automated, maintaining consistent CTTWD stabilizes deposition rates.

This concept is not new. Decades before the latest technologies arrived to optimize deposition rates, pressure vessel fabricators would take advantage of it. Many pressure vessels are fabricated from carbon steel but require a stainless steel overlay inside to protect the carbon steel from a corrosive environment. The SAW operators would swap the cables on the front of the power supply to change from DC+ to DC-. We know DC-, or straight polarity, produces the highest deposition rate and the lowest depth of penetration, which is what you want for an overlay application. They would then use an extended CTTWD of 3 or 4 in. to further increase the deposition rate based on the CA welding mode. This would allow them to weld perhaps two layers of deposit to attain the appropriate weld chemistry required for the application at a high deposition rate, saving a lot of time and money.

Technical Liaison

ESAB Welding & Cutting Products

Email Martin Denault

See More by Martin Denault

Senior Application Engineer, AWS – CWI, CWS, CWE

2800 Airport Road

Denton, TX 76207

See More by Robert Koltz

View the Digital Edition

Find The Welder on Facebook

Metal artist and fabricator Luis Varela-Rico joins The Fabricator Podcast to discuss his journey from union elevator mechanic…

Management FabCast Series 2026

FMA Annual Meeting 2027