We’re a small welding and fabrication shop that works in various industries. We mostly use gas metal arc welding (GMAW) and flux-cored arc welding (FCAW) to weld carbon steel. We recently started a job welding very thick sections of plain carbon steel. They are single-pass, 3/8-in. fillet welds performed in the flat position. We are using a 0.045-in.-dia. E71T1-1M wire preheated to 300 degrees F. However, we’re experiencing porosity with worm tracks and transverse cracking. Any thoughts on the cause?
Yes, there are a few potential causes for both issues.
Worm tracks are caused by the outer slag layer solidifying before the weld metal has solidified and completed its degassing phase. The chemical reactions taking place in a molten weld pool produce gases that must be allowed to escape prior to solidification to prevent the risk of porosity and worm tracks.
Porosity can happen with any type of welding process; however, worm tracks are unique to slag-producing processes like FCAW. This phenomenon is primarily unique to E71, similar filler metals, or, more specifically, all-position electrodes. The all-position electrodes produce a fast-freezing slag layer that allows welders to perform welds out of position, such as vertical-up or overhead. This fast-freezing slag system can pose a challenge with large welds in the flat or horizontal position. As mentioned, the slag layer solidifies before the weld metal and gases get trapped between the top of the weld pool and underside of the solidified slag.
Transverse weld cracks are generally associated with hydrogen, or what is termed hydrogen-induced cracking (HIC). Moisture in the filler metal introduces hydrogen into the weld pool via the flux, surface lubricants, weld joint contamination, atmospheric moisture, cutting fluids, etc. Four basic conditions must be present to have HIC: a susceptible microstructure, moisture source, tensile stress, and temperatures below 300 degrees F. Since you are welding on plain carbon steel, the likelihood of HIC is low. High-strength/low-alloy steels like A514, A517, chrome-moly, or nickel-chrome-moly steels are highly susceptible to HIC.
In your case, the transverse cracks may be caused by excessive internal porosity along with slag trapped at the root of the weld. In some cases, the combined effects can produce transverse cracks.
Using a 0.045-in.-dia. all-position electrode to perform a single-pass 3/8-in. fillet weld in the flat position is not recommended. The small-diameter wire requires weld transition dwelling to attain the proper size. What this means is the welder must transition very slowly and add in small pauses to allow the weld pool to spread out to attain the proper size. This technique allows weld metal to roll over the slag and trap slag at the root of the weld. Additionally, the welding arc will ride on top of the weld pool and act as an insulator to the underlying base metal, which prevents the welding arc from penetrating into the base materials and getting the required penetration. It is well documented that slag trapped at the root of the weld bead will act as a stress riser and lead to weld cracking. Also, if the throat of the weld is required to be 3/8 in., any slag at the root will reduce this dimension as well as the effective strength of the weld bead.
The electrode you are using requires a mixed gas such as C25—a 75% argon/25% carbon dioxide blend. Argon is a nonreactive gas and doesn’t provide the cleaning action in the weld pool like carbon dioxide does. This can also contribute to porosity, worm tracks, and reduced penetration—which combined can be the cause of your issues.
There are two simple ways to eliminate both of your issues. The easiest would be to change to a flat- and horizontal-only large-diameter electrode such as a 3/32-in.-dia. E70T-1C. This electrode type will have a slower freezing slag that allows gases to adequately escape, and the 100% carbon dioxide will provide improved cleaning action and penetration. The larger diameter will produce a wider arc and bead profile; the ability to handle higher currents will produce faster travel speeds due to higher deposition rates.
The other option is to perform the 3/8-in. fillet weld with a minimum of three weld passes and ensuring the welder stays on the leading edge of the weld pool. This will allow the weld pool to solidify at approximately the same time as the slag layer, reducing the tendency of worm tracks. Additionally, faster travel speeds will allow the welder to stay on the leading edge of the weld pool and attain proper penetration into the base material, preventing slag entrapment at the root. Always be sure to utilize a drag technique with any slag-producing filler metal to prevent slag entrapment at the root.
Technical Liaison
ESAB Welding & Cutting Products
Email Martin Denault
See More by Martin Denault
Senior Application Engineer, AWS – CWI, CWS, CWE
2800 Airport Road
Denton, TX 76207
See More by Robert Koltz
View the Digital Edition
Find The Welder on Facebook
Metal artist and fabricator Luis Varela-Rico joins The Fabricator Podcast to discuss his journey from union elevator mechanic…
Management FabCast Series 2026
FMA Annual Meeting 2027