The 20% rule can estimate the air-formed radius a press brake operator is likely to achieve, yet it remains imperfect. Data based on empirical evidence—test bends—can help most bending departments in metal fabrication shop. Phuchit / iStock / Getty Images Plus
Question: We bend a lot of stainless, mostly 11-ga., 7-ga., 0.25-in.-thick 300 series stainless. I was recently tasked with creating bend tables for SolidWorks, but unfortunately, I had to do so without coupon data. I began with the 20% rule, which you’ve written about at length. (Stainless forms an inside radius that’s 20% to 22% of the die width, 15% to 17% with 60-KSI mild steel). The rule seems to hold up for one material we have. Forming a grade of 0.375-in.-thick stainless over a 4-in. V die gives us a 0.750-in. bend radius.
So, I generated all our bend deduction tables using the 20% rule (21% for stainless), and our parts are now starting to hit the shop floor. But it appears that the 20% rule hasn’t held up too well there.
Forming 0.25-in. plate over a 2-in. V die gave us a radius of 0.420 in., or just 60% of our expected radius per the 20% rule. When we bent 7-ga. stainless over a 1.5-in. V die, we formed a radius of 0.315 in.—again, just 60% of the value we expected. When we bent 11-ga. stainless over a 1-in. V die, we achieved a 0.21-in. radius, or 74% of the expected value. Why did the 20% rule not hold up in our case?
Answer: To start, let’s review how air bending actually forms the inside bend radius. The punch forces the metal into a die, but unlike bottoming or coining, the punch does not bottom out in the die. The resulting bend radius is determined by a percentage of the die opening and the resilience, strength, and thickness of the material—and as you’ve discovered, it doesn’t always abide by rules of thumb.
When you air form a piece of sheet metal, the bend radius is not determined solely by the punch nose radius. Rather, the radius is a function of the die width. The punch doesn’t force the metal completely into the die, allowing it to spring back slightly after forming.
This relieving of the inside bend radius is known as a springback factor (Sf), and it can be calculated by dividing the outside bending angle—or the overbent angle that compensates for springback—and the bent angle, or the angle of the bend when it is released from pressure (see Figure 1).
For example, I might form to a bend angle of 92 degrees to achieve a 90-degree final bent angle. To determine Sf, you divide the bending angle by the bent angle:
Sf = Bending Angle/Bent Angle
Sf = 92/90 = 1.022
That value is multiplied by the original inside bend radius. Let’s say that your expected radius is 0.062 in.:
FIGURE 1. You form to the bending angle, after which the material springs back to its final bent angle
0.062 × 1.022 = 0.064 in.
In this case, 0.064 in. would be your working radius under perfect conditions and the value used to calculate your bend allowance and bend deduction.
The angular spread was 2 degrees, but it is not just 2 degrees. You must use the angles that are in play. Imagine you have two bends—one with an outside bending angle of 137 degrees and a bent angle of 135 degrees; another with an outside bending angle of 47 degrees and a bent angle of 45 degrees. Both have 2 degrees of springback, but they have different springback factors:
Sf = 137/135 = 1.014814
Sf = 47/45 = 1.0444444
Factors That Change the Radius
The bend radius in air forming is usually based on a percentage of the die opening, depending on the material’s properties. The bend radius can change for several reasons, even if you’re working with a consistent thickness and material type. One reason is, again, springback. Different die openings will result in different amounts of springback, which in turn affects the final bend radius. The metal’s elasticity allows it to spring back, which will be more or less pronounced based on the relationship between the punch and die dimensions.
Another reason the radius changes has to do with the material grain structure and internal stresses. This can alter the radius if the die opening changes.
When you increase the thickness of the same type of metal but keep the die size consistent, forming behavior changes. First, thicker metal has less springback because it’s stiffer and less elastic. It retains the deformation shape more than thinner metal.
Thicker material also increases your minimum inside bend radius to prevent cracking. Also, thicker material requires greater force to bend, which can lead to more pronounced deformation along the punch nose.
Meanwhile, if you decrease the die opening while maintaining a consistent material thickness, you increase the variations in bend angle, increase the tonnage requirements, and reduce the 20% rule’s accuracy.
FIGURE 2. The k-factor, expressed as t/Mt, is the ratio that describes the neutral axis’s inward shift during bending.
If the material is thick enough, the inside bend radius will begin to conform to the shape of the punch nose rather than floating as a percentage of the die opening. This happens for several reasons, one of them being the increased stiffness of thicker material. This makes it harder for the material to be shaped by anything other than the punch nose. As the material gets thicker, the influence of the die on the bend radius decreases. Also, thicker material has less elasticity, so it doesn’t “bounce back” as much and the radius becomes more defined by the punch profile.
So, what does this all mean? In essence, the bending radius in air forming is a dynamic relationship between material properties, thickness, die opening, and punch shape. With increased material thickness, this relationship changes, and the punch nose starts to play a more significant role in determining the bend radius, reducing the variability (or floating) of the radius relative to the die opening.